MULTIGRADE IV RC 
 
 
DISH/TRAY PROCESSING 
MULTIGRADE IV RC is processed in the same way 
as other resin coated papers. 
 
Note Photographic chemicals are not hazardous 
when used correctly. Always follow the health and 
safety recommendations on the packaging. 
Photochemicals material safety data sheets 
containing full details for the safe handling, 
disposal and transportation of ILFORD chemicals 
are available from ILFORD. 
 
 
Page 3 o
 
Processing summary (intermittent agitation) 
ILFORD Dilution 
ºC/ºF 
Time 
chemical (min:sec) 
Development 
MULTIGRADE 1+9  20/68  1:00 
or 
MULTIGRADE 1+14  20/68  1:30 
or 
BROMOPHEN 1+3 
20/68 
2:00 
or 
PQ UNIVERSAL   1+9 
20/68 
2:00 
Stop bath 
ILFOSTOP 1+19 
18–24/64–75 
0:10 
or 
ILFOSTOP PRO  1+19  18–24/64–75  0:10 
Fixation 
ILFORD RAPID  1+4  18–24/64–75  0:30 
FIXER or 
HYPAM 1+4 
18–24/64–75 
0:30 
 
Washing 
Fresh, running water  – 
Above 5/41 
2:00 
 
Development 
See the ‘Processing summary’ for development 
recommendations. 
 
On correctly exposed prints with MULTIGRADE 
developer 1+9, the image will begin to appear 
after 10 seconds. The minimum recommended 
development time for high quality prints is 45 
seconds; after this time there is a more gradual 
image build-up. Overexposed prints developed for 
a minimum of 35 seconds are acceptable for 
those applications where the highest quality is not 
required. 
 
To give greater control during development, and 
for economy, the 1+14 dilution of MULTIGRADE 
developer can be used. 
 
MULTIGRADE IV RC paper can also be processed 
in other high quality dish/tray developers. 
 
Stop bath 
See the ‘Processing summary’ for stop bath 
recommendations. 
 
The use of a stop bath is strongly recommended. 
A stop bath stops development immediately, 
reduces the risk of staining and will extend the life 
of the fixer bath. 
 
Fixation 
See the ‘Processing summary’ for fixing 
recommendations. 
 
The use of a hardening fixer is not recommended 
as it reduces washing efficiency. ILFORD RAPID 
FIXER and HYPAM are non-hardening fixers. 
 
There is no benefit in extending fixation beyond 
the recommended time; some loss of print quality 
might be seen when long fixing times are given 
due to image etching. 
 
Washing 
See the ‘Processing summary’ for washing 
recommendations. 
 
When it is important to obtain a print in the 
shortest possible time, vigorously wash 
MULTIGRADE IV RC paper for 30 seconds in 
running water. 
 
Prolonged immersion in water can cause edge 
penetration and print curl with resin coated 
papers: for this reason, avoid wet times longer 
than 15 minutes. 
 
Drying 
A final rinse in ILFORD ILFOTOL, diluted 1+200 
with water, will aid even and rapid drying. 
 
Optimum quality results will be obtained with the 
ILFORD series of dryers, for example, the ILFOLAB 
1250RC. 
 
When a dryer for resin coated papers is not 
available, remove surplus water from the prints 
and leave them to dry. At room temperature, prints 
will dry in 10–20 minutes. 
 
Note MULTIGRADE IV RC paper, as with other 
resin coated papers, should not be glazed/ 
ferrotyped or dried on a drum or flatbed glazer, 
as this can cause the polyethylene in the paper to 
stick to the glazing surface. 
f 4