Mercury Marine 899337001 ユーザーズマニュアル

ページ / 37
MAINTENANCE
29
Using 100 grit sandpaper or a pumice stone, roughen the patch
area  on  the  boat  as  well  as  the  backside  of  the  patch.  When
sanding, you just need to rub off the protective outer surface of the
fabric until a dull finish appears.
Clean the sanded surfaces with either toluene or tolual cleaning
solvents. Keep solvent off skin.
ONE PART GLUE (EMERGENCY REPAIRS ONLY)
Follow the directions on the cement tube.
TWO PART ADHESIVE
Mix a batch of adhesive according to the mixing directions provided
with the adhesive. Keep adhesive off skin. When the adhesive is
fully  mixed,  it  must  sit  for  a  short  time  to  activate  the  catalyst.
Failure to do so will create poor fabric adhesion.
Apply two thin layers of adhesive using a short bristle brush, in a
circular pattern on both the backside of the patch and the patch
area  on  the  boat.  Allow  the  first  layer  to  dry  completely
(approximately 15 minutes) before applying the second layer. The
second layer should dry until tacky, then apply the patch to the
prepared area and press down firmly. Using a smooth object (the
back of a tablespoon works well), force out any air bubbles that
may have been trapped under the patch, working from the center
of the patch to the outside.
After  removing  the  masking  tape,  use  solvent  to  clean  up  any
excess glue, then place a 4 ‑ 5 pound weight onto the patch and
allow  24  hours  drying  time  before  pressurizing  the  repaired  air
chamber.